TPE Trouble Shooting Guide

 Problem Possible Cause Possible Solution
Rough Surface Melt too cold Increase barrel temperature
    Increase die temperature
  Heaters not working Check thermocouples and heater bands
  Melt not mixed Use higher compression ratio screw or screw with mixing section
  Die design Decrease land length
Uneven Cross Section Surging Decrease extrusion rate
    Use screw with longer feed or metering section
    Use screen pack to increase back pressure
    Decrease die temperature
Black Specks / Undispersed Lumps Contamination Purge with low melt flow PP or HDPE
    Check the colour concentrate is based on PS,PP or PE - not PVC
Odor / Yellowing Melt too hot Decrease die and barrel temperature
    Decrease screw speed and back pressure
Voids Moisture Dry pellets
    If using vacuum check that vent is unplugged
High Extruder pressure / Low Throughput Melt too cold Increase extruder temperature
    Increase die temperature
  Clogged screen pack Clean/Replace
  Heaters not working Check thermocouples and heater bands


  Back